钛合金成分分析标准物质
(BT3-1)(BT9)
一、制备方法
真空自耗炉冶炼→浇铸成¢150m/m原锭→切头去尾、扒皮,进行偏析检验→机床车削、破碎→筛分选取 20~60 目→混匀→包装→均匀性检验→分析→数据汇总统计处理→定值
二、标准值及标准偏差
|
|
C |
Si |
Cr |
Mo |
AI |
Zr |
Fe |
N |
GBW02501 |
1 |
0.0140 |
0.278 |
1.568 |
2.565 |
6.145 |
0.270 |
0.480 |
0.0110 |
2 |
0.0130 |
0.267 |
1.552 |
2.542 |
6.452 |
0.285 |
0.475 |
0.0100 |
3 |
0.0125 |
0.288 |
1.560 |
2.540 |
6.378 |
0.285 |
0.459 |
0.0100 |
4 |
|
0.288 |
1.545 |
2.488 |
6.408 |
0.209 |
0.478 |
0.0094 |
5 |
0.0125 |
0.275 |
1.550 |
2.541 |
6.390 |
0.270 |
0.476 |
0.0080 |
6 |
0.0130 |
0.294 |
1.541 |
2.541 |
6.390 |
0.270 |
0.476 |
0.0100 |
标准值 |
0.013 |
0.28 |
1.55 |
2.53 |
6.42 |
0.276 |
0.473 |
0.010 |
标准偏差(S) |
0.001 |
0.01 |
0.01 |
0.03 |
0.04 |
0.012 |
0.008 |
0.001 |
GBW02502 |
1 |
0.0130 |
0.272 |
|
3.375 |
6.355 |
1.701 |
0.0682 |
0.0215 |
2 |
0.0120 |
0.267 |
|
3.362 |
6.312 |
1.700 |
0.0512 |
0.0215 |
3 |
0.0120 |
0.278 |
|
3.440 |
6.340 |
1.715 |
0.0518 |
0.0215 |
4 |
0.0122 |
0.278 |
|
3.390 |
6.308 |
1.692 |
0.0588 |
0.0195 |
5 |
0.0122 |
0.275 |
|
3.438 |
|
1.708 |
0.0572 |
0.0192 |
6 |
0.0122 |
0.280 |
|
3.423 |
6.315 |
1.720 |
0.0568 |
0.0220 |
标准值 |
0.012 |
0.275 |
|
3.40 |
6.33 |
1.71 |
0.057 |
0.021 |
标准偏差(S) |
0.0004 |
0.005 |
|
0.04 |
0.02 |
0.01 |
0.006 |
0.001 |
三、分析方法
元素
|
分析方法
|
C |
红外吸收法
|
库仑法(YB790-75)
|
Si
|
重量法(JIS H 1619-1978)
|
硅钼蓝光度法(BS-83045)
|
Cr
|
硫酸亚铁铵容量法(BS-83036)
|
Mo
|
硫氰酸盐萃取光度法(YB35(1-28)-78)
硫氰酸盐光度法(BS-83034)
|
Al
|
碱分离-EDTA 络合滴定法(BS-83053)
萃取分离-EDTA 容量法(YB769-70)
铬天青 S 光度法
|
Zr
|
偶氮胂Ⅲ光度法(YB35(16)-78)
EDTA 容量法(BS -83047)
|
Fe
|
邻菲啰啉光度法(BS-83046)
硫氰酸盐光度法(JIS H 1614-1970)
|
N |
蒸馏分离容量法(YB35-20-78) 蒸馏分离奈氏试剂光度法
|
四、均匀性检验
采用方差(F)检验法,检验结果(F<Fa) 样品均匀
五、包装、使用和贮存
瓶装、净重 50 克。称样后将瓶盖拧紧,存放于干燥处,严防氧化锈蚀。
注:以上信息仅供参考,以产品附带证书为准。